Published 26 November 2026 · Updated 26 November 2026

Epoxy bubbles: why they form and how to fix them

Temperature, mixing technique, seal coats and torch timing — everything that causes bubbles in a bar-top epoxy pour and how to prevent each one.

Bubbles are the most common complaint after a bar-top epoxy pour. The good news: nearly every bubble problem traces back to one of four causes, and each has a reliable fix.

The four causes and their fixes

Outgassing from wood

Porous wood releases trapped air as the epoxy heats up during its exothermic cure. This pushes tiny bubbles up through the coating for the first 30–60 minutes after the pour.

Fix: Always apply a thin seal coat first and let it cure 4–6 hours. The seal coat plugs the pores so the flood coat stays bubble-free.

Mixing too fast

Whipping the resin and hardener together whips air in. Those micro-bubbles are too small to rise out on their own before the epoxy starts to gel.

Fix: Stir slowly and deliberately for 3–4 minutes. Scrape the sides and bottom of the cup. After mixing, let the cup sit for 2 minutes before pouring — many bubbles will rise out in the cup.

Cold room temperature

Below 21 °C (70 °F), epoxy thickens and bubbles cannot rise to the surface before the resin gels. The result is frozen bubbles trapped in a cured but cloudy coating.

Fix: Keep the workspace at 22–27 °C (72–80 °F) throughout the pour and cure. Warm the resin bottles in a warm water bath (not above 40 °C) before mixing to lower viscosity.

No torch pass

Even with perfect prep, some bubbles will form. Without a heat source to pop them at the surface, they cure in place.

Fix: Pass a propane torch 15–20 cm above the surface in slow, sweeping motions. Do the first pass immediately after pouring, then repeat every 15 minutes for the first hour.

Torch technique

Hold the torch at an angle, not straight down. Keep it moving — a stationary flame scorches the resin and can cause yellowing or even ignite fumes in poorly ventilated spaces. Three to four passes across the entire surface is usually enough per round.

Tip: A heat gun set to low (around 120 °C / 250 °F) works as a safer alternative for small projects, though it takes longer. Avoid using a hair dryer — the airflow pushes dust into the wet resin.

What if bubbles have already cured?

If you find bubbles after the epoxy has hardened, sand the surface flat with 220-grit, clean off the dust and pour a fresh flood coat on top. The new layer bonds chemically to the sanded coat and gives you a second chance at a glass-smooth finish.

Sources

  1. West System troubleshooting guide
  2. TotalBoat epoxy FAQ and troubleshooting
  3. Epoxyworks issue on outgassing and bubbles
  4. Stone Coat Countertops bubble prevention tips